Test method for coating amount of PTP aluminum foil protective agent

The protective agent layer of PTP aluminum foil is a dense cross-linked resin layer formed by high temperature curing. It is difficult to completely wipe the coating in a short time by the solvent wiping method commonly used now, and it is difficult to obtain accurate coating quantity value. Moreover, the repeatability of sample test results is also very poor. Therefore, a more effective test method for the coating quantity of PTP aluminum foil protective layer is found, It is of great practical value to guide the production of such products.

According to the material characteristics of PTP aluminum foil and the comparison of the advantages and disadvantages of various detection methods, we finally believe that the "burning method" is the most suitable for the rapid detection of the amount of protective agent coating:

In this method, the PTP aluminum foil sample is placed in a muffle furnace, maintained at a certain temperature for a certain time, and the PTP aluminum foil coated with the protective agent layer is baked at high temperature, so that the protective agent layer is completely oxidized and gasified. The coating amount of the protective agent layer can be calculated by detecting the quality of the aluminum foil before and after the high-temperature baking.

1、 Instruments and reagents:

10cm * 10cm standard cutting plate, blade, analytical balance (precision: 1/10000 g), muffle furnace, glass plate, stainless steel tweezers, ethyl acetate (analytical pure), absorbent cotton

2、 Test method:

1. Select the aluminum foil sample sheet for drug packaging with flat surface and no wrinkles, cut 5 test samples with a blade and a 10cm * 10cm standard cutting plate, and control the deviation of the width and length of the sample within ± 0.5mm

2. Weigh the cut sample (W1) on the balance.

3. Put the printing face of the aluminum foil on a glass plate, and use stainless steel tweezers to clamp the degreased cotton dipped in ethyl acetate to wipe the heat-sealing coating surface of the aluminum foil until no obvious marks can be identified when the surface is observed with naked eyes. (Note: The cotton ball dipped with ethyl acetate shall not have the liquid of ethyl acetate dripping. The circular wiping method from the center to the edge shall be used for wiping. The edge of the aluminum foil must be laid flat on the glass plate, and the linear wiping method shall be used for wiping. The other side of the aluminum foil shall not be affected during the whole process as much as possible). If the cotton ball has been wiped with the printing coating, replace it with a new cotton ball.

4. After wiping the heat-sealing coating, put the aluminum foil in a ventilated place and place it at room temperature for 2 minutes.

5. Then weigh the weight (W2) on the analytical balance

6. Place the above aluminum foil on the sample shelf in the muffle furnace preheated to 550-600 ℃. After waiting for a period of time, take out the coated aluminum foil and place it at room temperature. (The black ink may not completely volatilize the pigment, and its impact can be temporarily ignored for the products with general printed text patterns. If the printed patterns are large, the weight impact of the ink binder and the pigment should be considered)

7. Then weigh the weight (W3) on the analytical balance

Note: If the test sample has no adhesive layer, omit the operations in 2, 3 and 4.

8. Result calculation:

(W1-W2) × 100=weight of heat seal layer (g/m2)

(W2-W3) × 100=weight of printing layer/protective layer (g/m2) (when the sample has adhesive layer)

(W1-W3) × 100=weight of printing layer/protective layer (g/m2) (when the sample has no adhesive layer)

W3 × 100=weight of aluminum foil layer (g/m2)

Calculate and report the test results and average values of all individual samples to the nearest 0.01g/m2.


主站蜘蛛池模板: 国产女精品视频网站免费| 亚洲精品欧美精品日韩精品| 调教套上奶牛榨乳器喷奶水| 狂野欧美性猛交xxxx| 无码人妻久久一区二区三区蜜桃| 天天躁日日摸久久久精品| 天天综合天天做天天综合| 国产日韩av免费无码一区二区| 无码少妇一区二区三区浪潮av| 黑色丝袜脚足国产在线看| 无码中文字幕在线播放2| 少妇伦子伦精品无码styles | 欲求不满邻居的爆乳在线播放| 精品一区二区的区别| 2020天堂在线亚洲精品专区| 插一插射一射视频| 亚洲欧美日韩精品久久| 天天做天天躁天天躁| 亚洲制服 视频在线观看| 午夜私人成年影院| 2021久久天天躁狠狠躁夜夜| 精品国产乱码久久久人妻| 亚洲人精品午夜射精日韩| 亚洲男人第一av网站| 久久不卡国产精品无码| 熟妇人妻不卡无码一区| 久久无码国产日本欧美| 亚洲精品第一国产综合亚av| 中文字幕丝袜精品久久| 亚洲—本道 在线无码| 成人h无码动漫在线观看| 国产做无码视频在线观看| 亚洲精品无码久久久| 失禁大喷潮在线播放| 国产小便视频在线播放| 小说区 综合区 首页| 国产丝袜在线精品丝袜| 夜色福利站www国产在线视频| 亚洲午夜福利在线视频| 久久久精品国产sm调教网站| 久久久精品人妻一区亚美研究所|